INTRODUCTION
During routine percentage-based non-destructive testing (NDT) using Magnetic Particle Inspection (MPI) on a deck crane’s slew hex nuts, fatigue crack-like indications were detected. This required further analysis to determine the nature of the defects.
BACKGROUND
Clients frequently send a sample percentage of slew fasteners to ALATAS for inspection and re-certification. Standard procedures include visual inspection and MPI to identify any abnormalities. In most cases, fasteners pass inspection and are returned to service. However, in this instance, crack-like defects were found. Since only a sample was tested while the remaining fasteners remained installed, the crane was taken out of service pending further investigation, making the job time-sensitive.
ALATAS’ SOLUTION
A more in-depth analysis was conducted. MPI was repeated to pinpoint the exact locations of the crack-like indications, which appeared on the non-load-bearing surface. The hex nuts were then cross-sectioned at these points for further examination. A stereoscopic analysis revealed that the cracks propagated parallel to the surface after initial entry—a characteristic of forging laps, a manufacturing defect.
Findings showed no evidence of further crack propagation during service life, and no abnormalities were detected on the load-bearing surface. As a result, the hex nuts were deemed fit for continued use, allowing the crane to be reinstated.
JOB SCOPE
- Standard NDT of slew hex nuts identified abnormalities.
- The crane was taken out of service for further investigation.
- More advanced testing was conducted on several hex nuts.
- The defects were confirmed to be a manufacturing issue rather than fatigue failure.
- The nuts were deemed safe for continued use, and the crane was reinstated.